Intumescent coating design is the engineering process of deciding which tested coating system protects each steel member, and at what dry-film thickness, so that the member keeps its load capacity for the fire-resistance period the building requires. It is not a paint choice made on site. In Dubai it starts with the required rating, runs through the steel section properties and the manufacturer’s certified data, and ends with drawings that the authorities accept and an inspection regime that proves the installed film matches the design.
This guide explains that sequence for developers, contractors and consultants who need exposed steel to meet Dubai requirements without losing the architectural intent of the structure.
TL;DR
- Intumescent coating swells under heat into an insulating char, which keeps structural steel below its critical temperature for the rated period.
- Thickness is never a rule of thumb: it is read from the manufacturer’s certified tables using the fire rating, the section factor and the critical steel temperature.
- Under Dubai Administrative Resolution No. (37) of 2021, the fire-resistance period is set by building type, use, hazard assessment and occupancy, and is not less than two hours for buildings generally.
- Primer, intumescent layer and topcoat must be a compatible, approved system, and the dry-film thickness must be measured and recorded after application.
- Coating decisions belong in the structural design stage, because they change member sizes, cost and the authority submission.
Table of Contents
- What intumescent paint does to steel in a fire
- How the required fire resistance is set in Dubai
- The design inputs that drive thickness
- How thick is intumescent paint in practice?
- Choosing the coating system
- Documenting the design for submission
- Application and inspection on site
- Our perspective
- Working with Integra on fire-protected steel
- FAQ
- Sources
What intumescent paint does to steel in a fire
Steel loses strength as it heats, and an unprotected section can reach its critical temperature in a matter of minutes. An intumescent coating reacts to heat by swelling in a controlled manner, producing an insulating carbonaceous char that slows the temperature rise in the steel beneath it. Research on intumescent coatings for steel structures describes this char as the mechanism that protects steel from high temperatures and damage, and notes that a complete system includes an anticorrosive primer and generally a topcoat.
The reason designers choose it is largely visual. The same research observes that intumescent coatings are often used when the architectural and aesthetic features of a steel structure should be preserved. A thin film can follow the profile of an exposed beam, a feature column or a roof truss, which sprayed cementitious fireproofing cannot do without changing the look of the member.
That benefit has a price. According to the AISC guidance on finishes, coatings and fire protection, intumescent coatings are generally more expensive than conventional spray-applied fireproofing, which is why they are typically used strategically on exposed, aesthetically sensitive members rather than across a whole building. In practice, a sound design mixes methods: concealed steel gets the economical option, and visible steel gets the coating.
How the required fire resistance is set in Dubai
The design begins with a number the designer does not choose. Under Dubai Administrative Resolution No. (37) of 2021, a building’s fire-resistance rating is based on its type, use, hazard assessment and occupancy, and the period must not be less than two hours for buildings generally. Fire-protection details must appear in the relevant drawings and satisfy the concerned authority.
The same resolution says the type of fire protection for steel is determined by several factors together: the required fire-resistance period, the specific protection system used, the perimeter of the steel section exposed to fire, the size of the steel section, and the building’s use or occupancy. In other words, the regulation itself points to the inputs of an intumescent design. A coating cannot be specified from a rating alone.
Two further requirements shape the workflow. Structural steel must be designed to the latest editions of American, European or British standard codes and specifications, and proposed fire-protection products and systems must be inspected by Dubai Central Laboratory or accredited laboratories under the adopted codes and standards. A product that carries only a foreign brochure is therefore not enough: its approval status has to be confirmed before it appears on a submission. Our guide to Dubai Civil Defence fire and life safety approvals for structural steel protection walks through how this fits the wider approval route, and our overview of the UAE Fire and Life Safety Code and building design covers the code context.
The design inputs that drive thickness
The question readers most often type is how thick intumescent paint should be. The honest answer is that it depends on the member, and the inputs are well defined.
Fire-resistance period
A 30, 60, 90 or 120 minute rating corresponds to progressively higher coating thickness, but not in a fixed ratio. A UAE coating supplier’s service page on intumescent paints states explicitly that the actual dry-film thickness must be read for each member from the specified system’s certified loading table, using the section factor and the critical steel temperature.
Section factor
The section factor is the ratio of the fire-exposed steel surface area to the steel volume, often written Hp/A and expressed in m⁻¹. A 2025 survey of commercial intumescent coating performance explains that specimens with lower section factors take longer to heat, and that section shape and fire exposure affect measured performance. Put simply, a heavy column warms slowly and needs less coating than a slender angle or light purlin carrying the same rating.
Critical temperature
The critical temperature is the steel temperature at which the member can no longer carry its load in the fire situation. It depends on how heavily the member is utilized: a lightly loaded beam tolerates a higher temperature than one working near its capacity. This is where structural analysis and fire design meet. Reducing member utilization, for example by choosing a heavier section, can raise the critical temperature and cut coating thickness, and that trade is a value engineering decision rather than a coating one.
A worked example
The 2025 survey gives a concrete case: an H-column requiring 60 minutes at a design temperature of 500°C and a section factor of 120 m⁻¹ needs 1.039 mm of dry film for the specified tested coating system. Change any one of the three inputs and the answer changes. The figure also applies only to that coating, which is why it cannot be borrowed for another product.
How thick is intumescent paint in practice?
Readers want a typical range, and one can be given if it is treated as orientation rather than specification. Thin-film coating thickness can range from well under a millimeter for short ratings to several millimeters for two-hour work, according to a fireproofing contractor’s guide to dry-film thickness factors, which also warns that a one-size-fits-all thickness is a critical error.
The 2025 survey of 62 commercial coatings adds useful context on chemistry: thin-film water-based and solvent-based systems are often certified below 1 mm, while epoxy-based systems generally require greater dry-film thickness. Both sources reach the same conclusion that matters for design: the required value must come from the manufacturer’s certified fire-resistance data for the specific member, not from a generic rule.
The thickness tables used in practice are derived from test results under EN 13381-8, as described in the academic review of coatings for steel. Product data sheets follow the same logic. The data sheet for Hempafire Pro 315, for instance, states that film thickness depends on the required fire resistance and the element’s massivity factor, and that the product is third-party certified to EN 13381-8 and optimized for R30 and R60. A product optimized for 30 and 60 minutes tells the designer something real: it is a natural fit for the lower ratings, and a two-hour requirement may point to another system or to a different protection method.
Choosing the coating system
The lowest thickness is not automatically the best outcome. The 2025 survey cautions that substrate, fire conditions, exposure, application method and certification range also govern selection. We use the following questions when a steel package reaches us.
Where will the steel sit?
Interior, conditioned steel in a dry atrium is a different environment from a car park, a plant room, a façade-adjacent column or a canopy exposed to Gulf humidity and salt. Durability classification and the type of topcoat follow from this. Dubai’s resolution also requires that proposed maintenance systems, such as galvanizing and protective paint, be considered when choosing corrosion protection, so the fire coating and the corrosion scheme should be designed together rather than by two parties who never meet.
Is the primer compatible?
The primer, the intumescent layer and the topcoat are tested as a system. Substituting a cheaper primer on site can void the certification. The same applies to galvanized steel: one manufacturer’s FAQ on its intumescent product says it can be used over galvanized steel if the substrate is suitably primed and the fire rating can be achieved, and that only primers and topcoats evaluated and approved by the manufacturer for compatibility, adhesion and fire performance should be used. Treat galvanized substrates as a specific item to confirm in writing with the supplier, not an assumption.
Is it approved for Dubai?
Because proposed products must be inspected by Dubai Central Laboratory or accredited laboratories, approval status belongs in the specification and the submission. Standards also matter: products certified to EN 13381-8 sit comfortably with the European, British and American code options the resolution allows, but the test basis should be stated on the drawing.
Should it be coating at all?
Sometimes the right answer is not intumescent. If steel will be concealed behind boards or finishes, a cheaper method may do the job. If the rating is long and the members are slender, coating thickness may become impractical and encasement or a heavier section may be better. A design review at concept stage settles this before procurement.
Is the signage and egress layout coordinated?
Exposed protected steel often runs along escape routes and beside fire exits, so the finish, the clearance and the safety signage should be planned together. For the signage side of that coordination, see this guide to fire safety signage compliance.
Documenting the design for submission
A coating design that cannot be read by a reviewer will slow approval. The package we expect to see, and prepare for clients, typically contains the following in prose form: a schedule giving each member mark, its section factor, the required rating and the critical temperature assumed; the specified coating system with its certification basis; the dry-film thickness for each member taken from the certified table; and a note on the maximum thickness the coating is tested for. Fire-protection details then go onto the relevant drawings, as the resolution requires.
This schedule also serves the contractor. The European industry good-practice guide for application, published by coating manufacturers and applicators, states that different sections may require different thicknesses and that each section should be identified for application and records. A clear member schedule makes that identification possible on site, and it makes the later inspection meaningful.
Our articles on steel structural design in Dubai under Dubai Municipality regulations and the structural inspection checklist for Dubai reviews show how these documents sit alongside the rest of the structural submission.
Application and inspection on site
Design intent is only realized if the film is applied as specified. Four checks matter most.
First, the environment during application. Temperature, humidity, ventilation and substrate condition affect application and cure, and the product data sheet states the limits. In Dubai summer conditions, this is a scheduling issue for enclosed or shaded work areas.
Second, the gauge. One manufacturer’s application manual for a thin-film system calls for the dry-film thickness gauge to be calibrated following ISO 2808:2001 and the manufacturer’s instructions.
Third, the acceptance method. The same manual records and confirms thickness using AWCI Technical Manual 12B or SSPC-PA2, and requires that it does not exceed the maximum fire-tested thickness for the member’s type, orientation, use and geometry. This second limit is often missed: a coating applied too thick is not a safer coating, because it falls outside what was tested.
Fourth, the records. Dry-film thickness is measured after application and logged against member marks, which is why the schedule described above matters. Where thickness readings fall short, the remedy is additional coat and re-measurement, not a note in the handover file.
An independent supervisor who reads the stamped drawings and the certified tables can catch these problems early. Our piece on construction supervision quality assurance against stamped structural drawings describes that role.
Our perspective
We see intumescent coating treated as a late procurement item far more often than as a design decision, and that is where projects lose time and money. When the rating, section factors and critical temperatures are fixed during structural design, we can balance heavier sections against thicker coating, group members sensibly and avoid specifying a two-hour system on members that could meet the requirement another way. When the coating is chosen after the steel is detailed and fabricated, the only variable left is thickness, and the cost goes up.
Our approach combines structural analysis to the codes the Dubai resolution recognizes with early engagement on the Dubai Municipality and Civil Defence submission, so that the coating specification, the drawings and the site inspection plan tell one consistent story. We would rather a client hears early that a particular member should be encased or resized than discover it during review.
— Aman
Working with Integra on fire-protected steel
Integra Consulting Services designs steel, concrete and other structures for projects in Dubai, the wider UAE and Saudi Arabia, and manages the authority route that follows. For steel packages that need coating schedules coordinated with member design, our steel structure design service and our Dubai Municipality and DDA submission support cover the structural analysis, the approvals management and the site supervision in one engagement. To discuss a specific building, start from the Integra services overview.
FAQ
Can intumescent paint be applied to galvanized steel?
Sometimes, but only as a verified system. One manufacturer states that its product can be used over galvanized steel when the substrate is suitably primed and the fire rating is achievable, using only primers and topcoats the manufacturer has approved. Get that confirmation in writing for the specific product before it goes into the specification.
How thick is intumescent paint on steel?
Thin-film coatings range from well under a millimeter for short ratings to several millimeters for two-hour work. The 2025 survey of commercial coatings gives a worked case of 1.039 mm for 60 minutes at 500°C and a section factor of 120 m⁻¹, but that figure belongs to one tested system. Your design thickness comes from the certified table for the chosen coating.
What fire rating does a building in Dubai need?
It depends on building type, use, hazard assessment and occupancy. Dubai Administrative Resolution No. (37) of 2021 sets the period at not less than two hours for buildings generally. Your structural engineer and the Civil Defence submission confirm the rating for your specific building.
Who checks the coating after it is applied?
The applicator measures dry-film thickness and records it by member, and the project supervisor or consultant verifies those records against the design schedule. Gauge calibration and acceptance follow the manufacturer’s stated standards, and the film must not exceed the maximum tested thickness.
Sources
- Intumescent Coatings for Fire Resistance of Steel Structures (MDPI, Coatings)
- Administrative Resolution No. (37) of 2021 Amending the Bylaw, Dubai Legislation
- A survey of commercial intumescent coating performance
- Intumescent coatings review, thickness tables and EN 13381-8
- Hempafire Pro 315 product data sheet
- Intumescent paints service page, UAE
- Intumescent coating DFT, cure time and performance factors
- Finishes, Coatings, and Fire Protection, AISC
- Firetex FX7002 Application Manual
- European industry best practice guide on the application of intumescent coatings
- Top 10 SteelMaster FAQs, Jotun
- Fire safety signage manufacturing: a compliance guide